\n
\u900f\u5c04\u955c\u7247\u6750\u6599 \u2014\u00a0\u6c1f\u5316\u94a1Barium Fluoride (BaF2)<\/p>\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n\n
Transmission Range<\/td>\n | 0.14 \u2013 14 (thickness 2mm)\u00a0\u00b5m<\/td>\n<\/tr>\n |
Refractive Index<\/td>\n | 1.47326 @633 nm<\/td>\n<\/tr>\n |
Reflection Loss<\/td>\n | 3.4% @4 \u00b5m;<\/td>\n<\/tr>\n |
Residual Beam Wavelength<\/td>\n | 47 \u00b5m<\/td>\n<\/tr>\n |
Density<\/td>\n | 4.89 g\/cm3<\/sup><\/td>\n<\/tr>\n |
Melting point<\/td>\n | 1368\u00b0C<\/td>\n<\/tr>\n |
Molecular Weight<\/td>\n | 175.36<\/td>\n<\/tr>\n |
Thermal Conductivity<\/td>\n | 10.9 W\/(m\u00b7K) @305K<\/td>\n<\/tr>\n |
Spec. Heat Capacity<\/td>\n | 410 J\/(kg\u00b7K)<\/td>\n<\/tr>\n |
Thermal Expansion<\/td>\n | 18.4 \u00b7 10-6<\/sup>\/K (273-573K)<\/td>\n<\/tr>\n |
Hardness (Mohs)<\/td>\n | 82 (load 500g)<\/td>\n<\/tr>\n |
Young\u2019s Modulus<\/td>\n | 53.07 GPa<\/td>\n<\/tr>\n |
Shear Modulus<\/td>\n | 25.4 GPa<\/td>\n<\/tr>\n |
Bulk Modulus<\/td>\n | 57.8 GPa<\/td>\n<\/tr>\n |
Fracture Modulus<\/td>\n | 26.9 MPa<\/td>\n<\/tr>\n |
Elastic Coefficient<\/td>\n | C11<\/sub>\u00a0= 91; C12<\/sub>\u00a0= 41.2; C44<\/sub>\u00a0= 25.3 GPa<\/td>\n<\/tr>\n |
Dielectric Constant<\/td>\n | 7.33 @f = 2 MHz<\/td>\n<\/tr>\n |
Solubility in Water<\/td>\n | 0.16 g\/100g @25\u00b0C<\/td>\n<\/tr>\n |
Crystal Structure<\/td>\n | single crystal, synthetic<\/td>\n<\/tr>\n |
Crystal Type<\/td>\n | cubic, CaF2 type structure, a=6.2\u00c5<\/td>\n<\/tr>\n |
Cleavage Planes<\/td>\n | (111)<\/td>\n<\/tr>\n |
Poisson Ratio<\/td>\n | 0.31<\/td>\n<\/tr>\n |
Application<\/td>\n | Scintillator, IR optics<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n
|